Technical Specifications

 

JOINING TECHNIQUE FOR PPR PIPES



 

PIPE WELDING

  1. Prepare the welding machine with the dies of the proper diameters to be processed, wait till the welding machine has reached the working temperature (260°C).
  2. Cut the pipe at right angle to the pipe axis. Remove burrs & chips.
  3. Mark the welding depth at the end of the pipe and fitting.
  4. Push the end of the pipe & fitting without turning, up to the marked welding depth into the welding tool. It is essential to observe the mentioned heating times.
  5. After the stipulated heating time quickly, remove pipe and fitting from the welding dies. Join them immediately, and without turning, until the marked welding depth is covered by the bead of PP-R from the fitting.
  6. The correction is only restricted to the alignment of pipe and fitting. Never turn the elements after the processing Time.
  7. Allow the cooling period.

 

RECOMMENDED TIME FOR FUSION WELDING

 

Pipe O.D.
mm
Insert Length  mm Heating up Sec. Processing
Sec.
Cooling
Min.
20 14 6 4 2
25 16 7 4 4
32 18 8 6 4
40 20 12 6 4
50 23 18 6 5
63 26 25 8 6
75 28 30 10 8
90 33 40 11 8
110 33 50 15 8

 